Carbon-Steel / Titanium Weld

PACE Technologies Etchant Database PACE Technologies Metallographic MET-MANUAL Link

Welding of disimilar metals can be challenging due to the individual properties, including melting temperatures and chemical compositions of the various metals. By analyzing the microstructure and the heat affected zone (HAZ), the quality, strength and properties of the metal interface can be examined.

SECTIONING

MAXCUT Abrasive blade (Cat. No. MAX-C or MAX-I series)

MOUNTING
Compression Mounting with Phenolic, Epoxy or Diallyl Phthalate compression mounting resins

POLISHING

Abrasive/surface

Lubricant

Force/ sample

Speed
(Head/base)

Time

120 micron diamond disk

Water

5-10 lbs

200/200 rpm

Until plane

9 um DIAMAT diamond on POLYPAD polishing pad

DIALUBE Purple Extender

5-10 lbs

200/200 rpm

3 minutes

3 um DIAMAT diamond on TEXPAN polishing pad

DIALUBE Purple Extender

5-10 lbs

200/200 rpm

3 minutes

1 um DIAMAT diamond on ATLANTIS polishing pad

DIALUBE Purple Extender

5-10 lbs

200/200 rpm

2 minutes

0.05 um Nanometer alumina on MICROPAD or MICROPAD 2 polishing pad

 

5-10 lbs

100/100 rpm

30 seconds


Metallographic micrograph of Welded Titanium to Carbon Steel.

Carbon-steel / Titanium Weld, 1500X, etched Sarajan's Reagent (73% DI water, 16% HF, 6% HNO3, 5% HCl)


Copyright © 2006-2017
PACE Technologies ® - 3601 E. 34th St. - Tucson, AZ 85713 USA
Telephone +1 520-882-6598 FAX +1 520-882-6599.
All Rights Reserved.


PACE Technologies facebook link   Blog us on Tumblr   Blog us on Tumblr   PACE Technologies Google+   PACE Technologies Google+   PACE Technologies Google+