Welding of disimilar metals can be challenging due to the individual properties, including melting temperatures and chemical compositions of the various metals. This is complicated more if one or more of the disimilar metals is a composite material. By analyzing the microstructure and the heat affected zone (HAZ), the quality, strength and properties of the metal interface can be examined.
SECTIONING
Diamond Wafering blade - medium grit / high concentration
MOUNTING
Castable Mounting with Epoxy or Acrylic resins
POLISHING
Abrasive/surface |
Lubricant |
Force/ sample |
Time |
30 um DIAMAT diamond suspension on CERMESH Metal Mesh cloth | 5 lbs | Until plane | |
6 um DIAMAT diamond on TEXPAN polishing pad | SIAMAT colloidal silica | 10 lbs | 5-10 minutes |
1 um DIAMAT diamond on ATLANTIS polishing pad |
SIAMAT colloidal silica |
10 lbs |
5 minutes |
SIAMAT Colloidal Silica on a TEXPAN polishing pad |
|
10 lbs |
5 minutes |
SiC-Titanium / Carbon-steel Weld, 200X, Etched Sarajan's Reagent |