Manganese Aluminum Bronze Specimen Preparation

Manganese-aluminum bronze is a relatively harder bronze because of the addition of manganese. Microstructural preparation of this material is relatively straight forward.

SECTIONING

MAXCUT Abrasive blade (MAX-C or MAX-I series)

MOUNTING
Compression Mounting with Phenolic, Epoxy or Diallyl Phthalate compression mounting resins

POLISHING

Abrasive/surface

Lubricant

Force/ sample

Speed
(Head/base)

Time

240 grit SiC paper
360 grit SiC paper
600 grit SiC paper
800 grit SiC paper
1200 grit SiC paper

Water

5-10 lbs

200/200 rpm

Until plane
1 minute
1 minute
1 minute
1 minute

6 um DIAMAT diamond on TEXPAN polishing pad DIALUBE Purple Extender

5-10 lbs

200/200 rpm

2 minutes

1 um DIAMAT diamond on GOLDPAD polishing pad

DIALUBE Purple Extender

5-10 lbs

200/200 rpm

2 minutes

0.05 um Nanometer alumina on NAPPAD polishing pad

 

5-10 lbs

100/100 rpm

1 minute


Metallographic micrograph of Nickel Iron Bronze

Mangnese-Aluminum Bronze, 400X DIC (etchant: ammonium persulface, HCl, DI Water)

About Us | Site Map | Web Disclaimer | Terms and Conditions | Contact Us
Copyright © 2006-2016
PACE Technologies ® - 3601 E. 34th St. - Tucson, AZ 85713 USA
Telephone +1 520-882-6598 FAX +1 520-882-6599.
All Rights Reserved.


PACE Technologies facebook link   Blog us on Tumblr   Blog us on Tumblr   PACE Technologies Google+   PACE Technologies Google+   PACE Technologies Google+